How to hot mount

Preliminaries to Mounting

image
  • Clean the Specimen
    The specimen should be cleaned before mounting in order to improve adhesion to the mounting medium. Use acetone or at least alcohol. Cleaning in an ultrasonic bath could be necessary. Remember to dry the specimen well. Clean specimens should be handled with either gloves or tweezers.
  • Adjust the specimen size to the cylinder size (~ 3.0-5.0 mm distance to cylinder wall).
  • Adjust the specimen height – the final height of the mount should be approx. 20 mm.
  • Select the most suitable hot-mounting resin.

Hot-mounting process

Two types of hot-mounting resin:

Selection of Resin / Selection Guide

The choice of resin/mounting media is very important in order to obtain the required result and fulfill the mounting requirements.

The purpose of this guide is to provide detailed information, hints and tricks about the various hot mounting materials. Go to Hot Mounting Selection Guide

Special applications Edge retention / general usage
Resin name

ClaroFast

CitoFast

ConduFast

PolyFast

DuroFast

LevoFast

PuriFast

MultiFast

Application

Transparence

Crystal clear mounts good for specimens with pores, voids or empty spaces. Can be used in a mixed mount as an insulator for electrolytical preparation or as a backfill for labelling.

Fast

Fastest hot mounting resin on the market. Best suited for soft materials or as "backing" for other resins when speed is of essence.

Conductive

Conductive resin relevant when electrolytical polishing and etching is used.

SEM analysis

Carbon filler enables SEM examination & offers very low shrinkage + high removal rate.

Edge retention

Superior edge-retention for hard & medium hard materials with very low risk of gaps.

Edge retention

Excellent edge-retention for medium hard & soft materials with very low risk of gaps.

Dust-free

No health hazards & dust free. Recommended for soft to medium hard materials.

Routine

Bakelite type resin for routine examination of soft to medium hard materials, or as backfill. Three colors available.

Shrinkage level Low Low Low Very low Very low Very low Medium Medium
Edge retention Fair Fair Fair Good Excellent Excellent Fair Good
Removal rate High High High High Low High High Medium
Mount hardness 81 Shore D 86 Shore D 76 Shore D 87 Shore D 86 Shore D 88 Shore D 62 Shore D 87 Shore D
Mounting time* (incl. heat-up) 10.5 min 3.5 min 5 min 5 min 5.5 min 5.5 min 5 min 5 min

Troubleshooting - hot mounting

Troubleshooting - hot mounting

image

Looking for consumables?

Order your consumables directly from our Webshop.

Visit the Webshop