Skip to content
Struers

Vickers Hardness Testing

The Vickers hardness test is suitable for a wide range of applications, including micro hardness testing. On this page, you can find a description of the Vickers hardness test, practical information on how to apply it and a list of our micro hardness testing machines for Vickers.

image

The Vickers hardness test at a glance:

  • Ideal for micro hardness testing
  • Can be used for case hardness depth measurement, Jominy testing and hardness testing of welds
  • Standards: ASTM E384, ISO 6507 and JIS Z 2244.
Find your next Vickers Hardness Tester

Definition of the Vickers hardness test

The Vickers hardness test is a versatile hardness test method, used for both macro and micro hardness testing. It has a broad load range, and is suitable for a wide range of applications and materials.

The Vickers hardness test is often regarded as easier to use than other hardness tests: The process can be performed on a universal or micro hardness tester; the required calculations are independent of the size of the indenter; and the same indenter (a pyramidal diamond) can be used for all materials, irrespective of hardness.

The Vickers Hardness calculation

The Vickers Hardness (HV) is calculated by optically measuring the diagonal lengths of the impression left by the indenter. The measurements are converted to HV using a table or formula.

  • Load range: From 10 gf up to 100 kgf

HV = 1854.4 F/d^2
HV: Vickers hardness
F: Test load (gf)
d: Average diagonal length (µm)

image

How to measure Vickers Hardness in 7 steps

Using a DuraVista-40 hardness testing machine:

  1. Place your sample on the stage.
  2. Click and drag the mouse to move the sample into position.
  3. Scroll to focus.
  4. Select the test method and load.
  5. Choose an objective and job name.
  6. Use the overview camera to position the indenter.
  7. Start the test.

Surface Preparation

Before placing the sample material in the micro hardness testing machine, you should ensure it is correctly prepared.

The required surface condition for the Vickers hardness test depends on the load used.

Macro hardness testing (loads higher than 1 kgf)

  • Surface should be ground

Micro hardness testing (loads below or equal to 1 kgf)

  • Surface should be mechanically polished or electropolished

Loads

STANDARD LOAD RANGE

ISO 6507

10 gf - ≤100 kgf

(0.0981 - 9.807 N)

ASTM E384

1 gf - ≤1 kgf
>1 kgf - ≤120 kgf

(0.0098 - ≤9.807 N)
(>9.807 - ≤1176.800 N)

  • Indentation time: 10-15 seconds
  • Sample thickness ASTM: At least 10 times the indentation depth
  • Sample thickness ISO: At least 1.5 times the diagonal length.

Download our Application note about Hardness Testing

image

Indent spacing

Regardless of the micro hardness tester you use, when you perform a Vickers hardness test, your indentation will deform the surrounding material and alter its properties. In order to avoid misinterpretations of perceived hardness, the Vickers hardness testing standards prescribe a certain distance between multiple indentations.

Steel and copper

  • At least 3 diagonal widths between indentations

Lead, zinc and aluminum

  • At least 6 diagonal widths between indentations

Diagonal widths

To ensure accurate reading of the indents, the Vickers hardness testing standards prescribe a minimum diagonal width of 20 µm.

For instance, this implies that CHD (see below) measurements using less than HV0.2 should generally be avoided, as they will produce indents smaller than 20 µm.

Vickers test methods and applications

Below you can see an overview of the Vickers hardness test methods and the most common applications:

TEST METHOD APPLICATION / MATERIAL

HV0.01
HV0.025
HV0.05

Small Geometrics, Thin Layers, Ceramics

HV0.1
HV0.25
HV0.3
HV0.5

Hardness Progressions, CHD/Eht-Nht-RHt

HV1
HV2
HV3

Hardness Progressions, CHD/Eht-Nht-RHt
Surface Hardness Testing
Surface Hardness Testing

HV5
HV10
HV20

Welding Test, Sintered Metals

HV30
HV50
HV100

Jominy Test, Surface Hardness Testing
Surface Hardness Testing
Surface Hardness Testing


Download our brochure covering our Vickers hardness testers

Case hardness depth (CHD) measurement

Surface Hardness

Hardness testing is often used to evaluate the hardness depth of surface-hardened steels. This is done by making a series of hardness impressions from the edge of the cross-sectioned sample towards the center. The hardness progression is plotted in a graph and the distance from the surface to the hardness limit (HL) is calculated.

When performing a hardness progression, it is important to observe the rules for indent spacing. Edge retention is also required during the mechanical preparation of samples to ensure an accurate measurement of CHD.

  • Case depth = Distance from surface to hardness limit

How to calculate CHD

There are different ways to determine the hardness limit. There are therefore different ways to calculate the CHD value. The procedure you choose depends on the hardening process used. The most common calculation methods are listed below.

1. Carburized or carbonitrided parts (EN ISO 2639)

  • Hardness limit = 550 HV
  • CHD (Eht) = Distance from the surface to the point where the hardness is 550 HV


2. Induction or flame-hardened parts (EN 10328 & ISO 3754)

  • Hardness limit = 80% x (minimum) surface hardness
  • CHD (Rht) = Distance from the surface to the point where hardness is 80% of the (minimum) surface hardness


3. Nitrided parts (DIN 50190-3)

  • Hardness limit = Core hardness + 50 HV
  • CHD (Nht, NCD) = (Maximum) distance from the surface to the point where hardness is 50 HV above core hardness


Example of CHD progression

  • CHD measurement displaying a CHD value of 0.95 mm at a hardness limit of 550 HV1
image
Different ways of calculating CHD

Comparison of Knoop and Vickers Hardness Testing

In most cases, the Vickers hardness test is used to determine hardness in materials in the micro hardness test load range. However, the Knoop hardness test is often used when hardness testing thin layers, such as coatings, or to overcome the problem of cracking in brittle materials.

When selecting which test to use, you should consider relevant standards, as well as the usual criteria when choosing between different types of hardness test.

Read more about Knoop Hardness Testing

image

Jominy testing

The Jominy test (End Quench Test) is a standardized test procedure used to determine the hardenability of steel, and it can be performed using any Vickers micro hardness tester.

  • The procedure is described in the following standards: ASTM A255 / ISO 642 / DIN 50191 / BS 4437

The Jominy test involves heating a cylindrical steel test piece to an austenitizing temperature (~980°–1010°C) and quenching (cooling) from one end, with a controlled and standardized jet of water. After quenching, the hardness is measured at intervals taken from the quenched end. The test method used is either HRC or HV30.

The hardness variation along the test surface is a result of microstructural variation that arises as the cooling rate decreases with the distance from the quenched end. The harder the material at a given distance from the end, the higher the hardenability of the steel.

Both the Vickers and the Rockwell hardness tests are often used for Jominy testing. When selecting which to use, pay attention to the relevant standards, as well as the usual criteria when choosing between different types of hardness test.

Find out more about the Rockwell hardness test

image
Jominy testing
image

Hardness testing of welds

Hardness testing of welds is a subgroup of the Vickers hardness test. The purpose of these hardness tests is to evaluate the strength of the weld, with particular focus on hardness around the heat-affected zone (HAZ). This is because the hardness in and around the HAZ can help evaluate the brittleness of the weld and can therefore help you determine whether or not the weld has the strength you require. Hardness testing of welds can be performed on any Vickers micro hardness testing machine.

When hardness testing of welds, a series of measurements are made in a given pattern at a specific distance from the sample edge or top of the weld. The progression of the hardness values can then be plotted in a graph.

  • Methods typically used: HV5 and HV10
  • Applicable standards: ISO 9015-1/-2
Download Weld Application Note

Downloads and webinars

Whether you're just starting with hardness testing or are an experienced professional, this curated selection of resources is here to assist you in your work.

Take advantage of downloadable reference posters for easy use in your lab, and dive into expert-led webinars hosted by our application specialists to deepen your understanding of hardness testing techniques and methods.